Parging a Foundation or Block Wall: Materials and Method
Parging is a thin coat of cement mortar troweled onto a masonry or concrete wall, most often the exposed part of a block or poured foundation. Above grade it gives a uniform, finished look and protects the mortar joints. Below grade, on a block foundation, it is the base that dampproofing goes onto. It is a straightforward DIY job if the wall is sound and the coat is applied and cured properly.
What parging is and is not
- It is a cosmetic and protective skin, usually about 3/8 to 1/2 in (10 to 13 mm) thick in total, applied in one or two coats.
- It is not waterproofing. Parging reduces water entry through a block wall, but cement mortar still absorbs water. For basement masonry walls, the International Residential Code calls for at least 3/8 in (9.5 mm) of portland cement parging on the exterior, followed by a dampproofing coating, unless a dampproofing product approved for direct application is used. Local codes vary; check yours.
- It is not a structural repair. Parging over a cracked or bowed wall hides the problem without fixing it. Wide cracks, cracks that keep growing, stepped cracks through the block joints, horizontal cracks, or a wall that leans or bows need a structural engineer to look before anything is covered up.
- It is not stucco. Stucco is a full wall cladding system, usually over lath on framed walls. Parging is applied directly to masonry or concrete.
Materials
- Mortar: premixed Type S mortar mix is a common choice. Bagged parging mixes and surface-bonding or resurfacing cements are also sold for the purpose; follow their labels. A site mix of 1 part portland cement, 1/2 part hydrated lime and about 4 1/2 parts sand by volume (a Type S proportion) also works. See mortar types.
- Bonding agent: an acrylic bonding agent or admixture helps on smooth poured concrete and on old parging. Do not parge over paint; remove it.
- Water and a garden hose or sprayer for dampening and curing.
How much mortar
Work out the area and thickness: length x exposed height gives square feet; multiply by the thickness in inches and divide by 12 to get cubic feet. Divide by the yield in cubic feet printed on your mortar bag, add about 10% for waste, and round up.
Example: a 40 ft (12.2 m) wall with 2 ft (0.6 m) showing, parged 1/2 in (13 mm) thick: 40 x 2 = 80 sq ft; 80 x 0.5 / 12 = 3.3 cu ft; plus 10% = about 3.7 cu ft. At a stated yield of, say, 0.6 cu ft per bag, that is 7 bags. Use your bag's own figure.
Tools
- Cold chisel, hammer, stiff wire brush, scraper
- Mixing tub and hoe, or a drill with a paddle
- Hawk and steel finishing trowel; margin trowel
- Scratching tool (a notched trowel, a scarifier or a few nails through a board)
- Sponge float or wood float, or a soft brush, for the finish texture
- Spade, for digging a few inches below grade
- Alkali-resistant gloves, goggles, long sleeves, respirator for chipping
Step by step
- Check the weather. Parge when the air and wall will stay above about 40 F (4 C) for at least a day or two and no frost is forecast. Avoid strong direct sun, hot wind and rain on fresh work; an overcast day is ideal.
- Dig down. Expose a few inches of wall below the soil line so the parging runs below grade and its bottom edge is not left exposed to splashback.
- Remove loose material. Chip off loose or hollow-sounding old parging. Wire brush the wall to remove dirt, efflorescence (white salt deposits) and anything flaking. Fix active leaks first; see hydraulic cement for plugging leaks.
- Dampen. Wet the wall thoroughly a while before you start and again just before each coat, so it is damp but without standing water. A dry block wall sucks water out of the mortar and the coat will not bond. Apply bonding agent now if you are using one, following its open time.
- Mix. Mix to a stiff, workable consistency that stays on the trowel and on the wall without sagging. Mix only what you can use in about an hour or so; do not add water to mortar that has started to set.
- Scratch coat. Press the first coat on firmly, about 1/4 to 3/8 in (6 to 10 mm) thick, working from the bottom up. When it has firmed slightly, scratch horizontal grooves across it to give the next coat a key.
- Let it firm. Wait until the scratch coat is firm but still damp, typically a few hours depending on weather. Mist it if it is drying fast.
- Finish coat. Dampen the scratch coat lightly and apply the second coat, about 1/4 in (6 mm), bringing the total to about 1/2 in. Trowel it flat. For a single-coat job on a sound, even wall, apply one coat of about 3/8 in or more and skip the scratching.
- Texture and top edge. When the surface has lost its sheen, finish with a sponge float, wood float or soft brush for an even texture. Bevel the top edge so water runs away from the wall and the sill plate, not into the joint behind the parging.
- Cure. Keep the parging damp for at least 2 to 3 days by misting it a few times a day, or cover it with damp burlap or plastic. Shade it from sun and wind. Parging that dries in hours cracks and comes loose.
- Backfill and dampproof. Once cured, apply any dampproofing coating the code requires on the below-grade part, then replace the soil, sloping it away from the wall.
Why parging fails
- Delamination (sounds hollow, falls off in sheets): wall too dry, dirty or painted, no bonding agent on smooth concrete, or one coat applied too thick.
- Map cracking: drying too fast; no curing; mix too wet or too rich in cement.
- Cracks that line up with cracks in the wall: the wall is moving. Parging will not stop that, and a moving crack in a foundation needs an engineer's assessment. See why concrete cracks.
- Flaking at the bottom: parging ended above grade or water is splashing and freezing there; extend below grade and fix drainage.
Safety
- Wet mortar burns skin. It is strongly alkaline, and burns may not hurt until hours later. Parging means a lot of hand contact and splashing; wear alkali-resistant gloves, long sleeves and trousers, and eye protection. Wash splashes off promptly with clean water and remove soaked clothing. If mortar gets in your eyes, rinse with clean water for at least 15 minutes and get medical help. Cement and lime can also cause allergic skin reactions, so wear gloves even on a small patch.
- Silica dust: chipping off old parging and wire brushing or grinding masonry releases respirable crystalline silica, which causes lung disease. Wet the wall while you work, use tools with on-tool dust extraction if you grind, wear a properly fitted respirator, and clean up with a HEPA vacuum or water, never by dry sweeping.
- Dust from bags: open and pour mortar and lime with a dust mask and eye protection, standing upwind.
- Lifting: mortar bags are often 80 lb. Lift with your legs, get help, use a barrow.
- Digging: locate buried utilities before you dig along a foundation.