Hydraulic Cement: Plugging Leaks in Concrete and Masonry
"Hydraulic cement" means two different things, and the difference matters when you are standing in a store aisle with a leaking basement wall.
- The technical meaning: any cement that sets and hardens by reacting with water, and can do so underwater. Portland cement is a hydraulic cement, and the US performance standard for cements, ASTM C1157, is titled for hydraulic cement. In this sense, almost all concrete is made with hydraulic cement.
- The product on the shelf: a bag labeled "hydraulic cement" or "water-stop cement" is a special fast-setting, expanding cement for plugging holes and cracks that are actively leaking. That is what this page is about.
How water-stop cement works
Water-stop cements set in minutes, fast enough to harden while water is still pushing through the hole. They also expand slightly as they harden, which locks the plug into the hole. The trade-off is a very short working time: one maker's instructions say to mix only what you can place within 2 to 3 minutes. They are rigid once set.
What it is good for, and what it is not
Good for
- Stopping active seepage through a crack or hole in a concrete or block basement wall or floor
- Sealing gaps around pipes that pass through a foundation wall
- Plugging form-tie holes and small holes in concrete tanks, pits and cisterns that are not used for drinking water (check the product's approvals for anything holding potable water)
Not a fix for
- The cause. Most basement leaks come from water around the foundation: gutters and downspouts emptying beside the wall, ground sloping toward the house, or blocked drains. Plugging the crack without fixing the water source often moves the leak to the next weak spot.
- Moving cracks. A rigid plug in a crack that still opens and closes will crack again beside it.
- Structural damage. Wide cracks, cracks that keep growing, stepped cracks in block walls, cracks where one side has moved out of line from the other, a bowing wall, or doors and windows above that have started to stick: these need a structural engineer to look before anything is patched. See why concrete cracks and which cracks matter.
- Whole-wall waterproofing. It plugs a point; it does not waterproof a wall.
Tools and materials
- Hydraulic water-stop cement (small tubs and bags are enough for most leaks)
- Cold chisel and hammer; wire brush
- Small mixing container, clean cold water, measuring cup
- Trowel or putty knife
- Alkali-resistant gloves, safety goggles, respirator (for chiseling), long sleeves
How to plug a leaking crack or hole
- Open it up. Chisel the crack or hole out so it is at least about 3/4 in (19 mm) wide and deep (one maker's minimum). Make the sides square or undercut, so the hole is wider at the back than at the surface. Avoid a V-shape: the expanding plug locks in only if the sides hold it.
- Clean it. Remove loose concrete, dust and old filler with a wire brush. Flush with water. The surface should be wet, which is normal for this product.
- Mix a small amount. Use the water ratio on the label (one product calls for roughly 4 parts powder to 1 part water) and mix to a stiff, putty-like dough. Mix only what you can place within the working time on the label, often 2 to 3 minutes. Never add more water to a batch that is stiffening; mix a fresh one.
- Press it in. Push the cement firmly into the opening with a gloved hand or trowel and hold steady pressure while it sets, typically a few minutes. For a running leak, some installers shape the cement into a plug and wait until it begins to stiffen before pushing it in, so the water cannot wash it out.
- Finish. Trim or smooth the surface flush with a trowel before it hardens fully.
- Cure and coat if needed. Keep the patch damp for the time the label states. Once cured, the wall can be coated with a masonry waterproofing coating if you want one.
- Fix the water. Extend downspouts away from the house, clean gutters, and regrade soil to slope away from the foundation. Watch the patch through the next wet season.
Related repairs
- A dry, non-leaking crack in a driveway or path is a sealant or repair mortar job. See how to repair cracks in a concrete driveway.
- Once leaks are stopped, the outside of a block foundation is often parged. See parging a foundation or block wall.
Safety
- Wet cement burns skin. Hydraulic cement is strongly alkaline, and you will be handling it with your hands. Wear alkali-resistant gloves; burns may not hurt until hours later. Wash any on your skin off promptly with clean water. It also warms up as it sets.
- Eyes: wear goggles, especially when chiseling or working overhead on a wall. If cement gets in your eyes, rinse with clean water for at least 15 minutes and get medical help.
- Silica dust: chiseling or grinding concrete and block releases respirable crystalline silica, which causes lung disease. Wet the area while you chip, wear a properly fitted respirator, and clean up with a HEPA vacuum or wet methods, never by dry sweeping.
- Dry powder: open and pour with a dust mask and eye protection; work with ventilation in a basement.
- Electricity: a leaking basement is a wet floor. Keep power tools and extension leads out of the water and use GFCI-protected outlets.